prosthodontics

Wol-Ceram Coping & Bridge

2007-10-15

Sintering and Infiltration of the Wol-Ceram Coping & Bridge
Sintering
The Wol-Ceram copings and bridges are fired in the oven for approximately 1-4 hours at 1120C, this procedure is called sintering.

Sintered Copings & Bridges

 

 
Infiltration
After the coping and bridge are sintered, the final step is infiltration. The Wol-Ceram copings and bridges are coated with an infiltration glass that comes in four different vita shades, and they are fired in the oven for approximately 1-4 hours at 1100C.

Infiltration Glass on Copings

 
 

After Glass Infiltrating

 

After Finishing

 

After Glass infiltration sandblast the copings with 50 um Al2O3 at a maximum pressure of 2.5 – 3.0 bar.

 

Copings are ready for veneering.

Venering and Cementation
The final veneering of the Wol-Ceram restoration is done following standard procedures with any of the porcelains currently available such as Vita Alpha, Vita VM7, Noritake Cerabien, Jensen Creation AV, Vintage AL Esthetic Porcelain, and All-Ceram.

The strength of the Wol-Ceram coping allows it to be cemented with conventional cements used for PFM restorations. In-Ceram restorations can be bonded using Panivia 21 TC, Rely X from 3M, or by using most conventional cements.